April_AMP_Digital
A D V A N C E D M A T E R I A L S & P R O C E S S E S | A P R I L 2 0 1 8 2 8 of the ceramic phase. High ductility is ascribed to strong interfacial bonding between the ceramic particles and the metal matrix. Tensile results at 400 o C (Fig. 4) show that flow stress increas- es from 10 MPa for pure Mg to 25 MPa for the composite. The mode of fracture changed from transgranular to inter- granular, which is expected for disper- sion-strengthened alloys. The stress rupture behavior of the composites was determined from creep tests at 350 o to 450 o C (Fig. 4) [17] . Further work on microstructure characterization and discussion of the strengtheningmechanisms is described in the literature [18-20] . SUMMARY The developing technology de- scribed in this article is poised to en- able the design and creation of a new generation of creep-resistant metal al- loys. Aluminum and magnesium are usually precipitation hardened; precip- itates are produced by diffusion in the solid state under controlled heat treat- ment. In high temperature creep, these same diffusion mechanisms lead to coarsening, which degrades creep resis- tance. PDC-MMCs contain particles that are inert and do not coarsen, thereby enabling a new generation of high-tem- perature metal alloys. Melding of polymers and metals to produce high temperature metal al- loys is unusual, and a concerted effort is needed to develop the technology. The organic precursors are nonflammable, nontoxic, and environmentally benign, posing little risk in scale-up to manu- facturing, although in some instanc- es, shielding with an inert gas may be needed because some of them convert into the ceramic if exposed to air. Thus, their incorporation into metallurgical processes is feasible. The opportuni- ties may be difficult to fathom today, but they are likely to be revolutionary. ~AM&P For more information: Rishi Raj is a mechanical engineering professor, Uni- versity of Colorado Boulder, 596 UCB, Boulder, CO 80309-0596, 303.492.1029, rishi.raj@colorado.edu, www.colorado. edu . Acknowledgment The results reported here are from the doctoral theses supervised by M. Surappa, Indian Institute of Science, H. Singh, Indian Institute of Technolo- gy, A. Molinari, University of Trento, It- aly, and the author. Post-doctoral work (Sudarshan) was supervised by the au- thor [12,13,20-24] . Doctoral research was car- ried out partially at University of Colo- rado Boulder, supported by the Metals and NanoMaterials Program in the NSF Division of Materials Research under Grant No. DMR1105347. References 1. W.H. Rhodes, Agglomerate and Par- ticle Size Effects on Sintering Yttria- Stabilized Zirconia, J. Amer. Ceram. Soc., 64, (1), p 19-22, 1981. 2. F. Dynys and J.W. Halloran, In fluence of Aggregates on Sintering, J. Amer. Ceram. Soc., 67 (9), p 596-601, 1984. 3. D.L. McDanels, Analysis of Stress- Strain, Fracture, and Ductility Behavior of Aluminum Matrix Composites Con- taining Discontinuous Silicon Carbide Reinforcement, Metall. and Matls. Trans. A, 16, (6), p 1105-15, 1985. 4. T.W. Gustafson, et al., Influence of Microstructural Scale on Plastic Flow Behavior of Metal Matrix Composites, Acta Materialia, 45, (4), p 1633-43, 1997. 5. B.A. Wilcox and A.H. Clauer, Creep of Thoriated Nickel Above and Below 0.5 TM, Trans. Met. Soc. AIME, April, p 236, 1966. 6. J. Hashim, et al., Metal Matrix Composites: Production by the Stir Fig. 3 — Effect of introducing polymer-derived ceramic particles into Mg by in-situ conversion of the organic precursor. The precursor can be injected directly as a liquid or powder of cross- linked polymer into molten magnesium; both give similar results. Fig. 4 — Results of creep tests carried out at 350 o to 450 o C: (left) effect of ceramic dispersion on the flow stress at a strain rate of 10 − 3 s − 1 ; (right) data fitted to the Monkman-Grant relationship.
Made with FlippingBook
RkJQdWJsaXNoZXIy MjA4MTAy