April_AMP_Digital
A D V A N C E D M A T E R I A L S & P R O C E S S E S | A P R I L 2 0 1 8 2 6 polymers at ~350 o C, which are relatively stable in air up to ~600 o C, but then decompose into ceramics. These fall into two subclasses, B1 and B2. • Type B1 includes silicones and silazanes that yield amorphous ter- nary ceramics constituted from Si, C, and N/O, which have the compo- sition SiCO (SiCN), and are inert and stable above 1200 o C. • Type B2 includes carbosilanes that yield binary SiC, which is normally nanocrystalline with some residual carbon at the grain boundaries. They are linear chain polymers built on silicon backbones, which can be drawn into fibers. The fabrication of in-situ PDC- MMCs is carried out by introducing the raw precursor into the metal matrix in a fine dispersion, followed by in situ con- version of the polymer into the ceramic phase by heating to between 700 o and 800 o C. If the melting point of the host metal is above the pyrolysis tempera- ture, the polymer must be introduced by milling the metal powders with the polymer powders, followed by hot con- solidation with traditional powder metallurgy methods. The polymer py- rolyzes during hot consolidation of the powders. This approach is used with a Cu metal matrix. If the metal melts below 700 o C, the polymer can be introduced directly into the molten metal either by injecting the liquid polymer directly into the melt, or by injecting the cross-linked powder of the polymer precursor into the melt. This approach is used with a Mg metal matrix. Excellent wetting of the poly- mer powder enables having it drawn spontaneously into the melt. POWDER-METALLURGY ROUTE Copper-SiCN MMCs [12, 13] were pre- pared by cryomilling powders of cross- linked commercial polysilazane (Type B1) to a 0.5 to 30-µm particle size with 60 to 100-µm copper powder. Ceram- ic yield from the polymer ranged from 80-90 wt%. Two-step milling was used to produce samples with 3.5, 6, 10, and 12 vol% ceramic phase (A3, A6, A10, and A12), respectively, as well as a high volume fraction composite (B30) con- taining 30-35 vol% PDC. Figure 1 shows an electron micrograph of the milled powder and of the MMC after hot con- solidation. Milling led to significant grain refinement (50-130 nm) in the metal. Microindentation hardness mea- surements show a linear relationship between the microhardness (which is proportional to the yield stress) and (1/ λ ), as predicted by Equation 1 for a given particle size. The main effect of higher volume fraction of a ceram- ic phase is a reduction in interparticle spacing. Polymer-derived ceramic par- ticles that form are inert and therefore do not coarsen, even at high tempera- tures. Figure 2b confirms the stability of the ceramic particles, showing that (b) (a) Fig. 1 — Composites made with Cu powder and cross-linked Type B1 precursor, milled and hot consolidated: (a) TEMmicrograph of milled powder, and (b) hot-consolidated sample contain- ing 30-35 vol% ceramic phase. The length of the interspersed nanostructure of the metal and ceramic phases is about 100 nm. Fig. 2 — Casting made by injecting powder of Type B1 precursor into Mg melt: (a) optical micrograph shows ceramic particles segregate to grain-boundary regions; (b) SEMmicrograph after hot extrusion; (c) Raman spectra show D and G peaks of graphene, which confirm full conversion of the precursor into the ceramic phase; and (d) compression creep behavior of pure sample and extruded sample shown in (b). (b) (a) (d) (c)
Made with FlippingBook
RkJQdWJsaXNoZXIy MjA4MTAy