April_AMP_Digital

A D V A N C E D M A T E R I A L S & P R O C E S S E S | A P R I L 2 0 1 8 2 5 INTRODUCING NANOSCALE CERAMIC PARTICLES INTO METAL MATRICES Melt-injection of organic precursors may result in revolutionary technologies for producing ceramic reinforced metal-matrix composite castings. Rishi Raj University of Colorado, Boulder S intering is used to fabricate ceram- ics with high melting points, where densification occurs by solid-state diffusion. The high sensitivity of sintering rate to particle size [1] led to commercial development of fine nanometer-scale ceramic powders. Van der Waals forces cause the fine powders to form hard par- ticles [2] , which have gained consideration for use as reinforcements inmetal-matrix composites (MMCs). High volume fractions of ceramics enhance the modulus of the composite, which depends mostly on the volume fraction of the ceramic phase. This con- cept is applied to SiC-reinforced alu- minum matrix composites [3] . However, enhancement of yield strength and creep resistance requires nanoscale dispersion of the ceramic particles, which is approximately given by the Orowan stress: (1) where σ y is shear yield stress, G is shear modulus, b is the Burgers vector (essentially equal to the lattice param- eter), and λ is the interparticle spac- ing. Therefore, to achieve a yield stress that is 1%of G requires that λ is equal to roughly 100 times the lattice parameter (~15-20 nm). Assuming the particles are in the form of cubes (different particle shapes lead to minor differences in a numerical factor) of size p , the spacing between adjacent particle edges is giv- en by [4] : (2) For example, λ is equal to 4 p for a volume fraction ( f v ) of 0.01. If λ = 20 nm, the particle size must be just a few tens of nanometers. The influence of par- ticle dispersion on creep resistance is more complex, but essentially follows a similar guideline. If particles coars- en at elevated temperatures, such as with precipitation-strengthened alloys, creep resistance degrades with increas- ing particle size. Therefore, inert parti- cles, which have little or no solubility in the metal matrix, are required for good creep resistance. ODS alloys made of nickel and thoria particles by deforma- tion processing are an example of such optimized design of MMCs [5] . Thus, the goal in creep-resistant MMCs is to be able to disperse essen- tially inert nanoscale ceramic particles. One approach has been to mix readily available fine ceramic particles into a metal by mechanical methods. Howev- er, the fine particles form hard agglom- erates, which must be broken down by mechanical stirring. Ultrasonic meth- ods have been used, but have yet to show commercial potential [6] . Process- es where second phases are produced by in-situ reactions with the host met- al have also been explored [7] . This work differs in that the chemistry of the ce- ramic phase is contained entirely within the organic precursors, which imparts simplicity and versatility to the poly- mer route. WHY THE POLYMER ROUTE? Conversion of organics into ce- ramics is a relatively new field [8] . Typ- ically, organics convert into ceramics at low temperatures in the range of 400 o to 800 o C, increasing the possibili- ty of in-situ production of fine ceramic particles within a metal matrix. The or- ganics are self-contained, i.e., they de- compose by themselves to produce the ceramic without needing to react with the metal host. There are two class- es of the organics (generally known as polymer-derived ceramics, or PDCs): volatile (generally called alkoxides [9] ) and those that remain in a condensed state until converting into the ceramic phase [10, 11] . PDCs include: • Type A are usually liquid at am- bient temperature, but develop significant vapor pressure above ~400 o C. Vapor pressure depends on monomer molecular weight; larger hydrocarbon side groups increase molecular weight and lower vapor pressure. These yield oxides. • Type B have networks like oligomers (large 3D molecules built around silicon) or linear chains made of Si backbones. These nonvolatile com- pounds cross-link into epoxy-like

RkJQdWJsaXNoZXIy MjA4MTAy