April_AMP_Digital
A D V A N C E D M A T E R I A L S & P R O C E S S E S | A P R I L 2 0 1 8 2 1 large aircraft company has its own set of alloy specifications. The alloy name in the U.S. can include a company name or trademark in conjunction with the alloy composition or strength, i.e., ul- timate tensile strength for TIMET and yield strength for other U.S. producers, for unalloyed titanium. Because titanium alloys are used in a variety of applications, several dif- ferent material and quality standards are specified. Among these are ASTM, ASME, Aerospace Materials Specifica- tions (AMS), U.S. military, and a num- ber of proprietary sources. The correct chemical composition is basic to ob- taining mechanical and other proper- ties required for a given application. Mi- nor elements controlledby specification include carbon, iron, hydrogen, nitro- gen, and oxygen. In addition, control of thermomechanical processing and subsequent heat treatment is vital to obtaining the desired microstructure and mechanical properties. In criti- cal applications, such as rotating parts in aircraft gas turbines, raw materials, melting parameters, composition, ther- momechanical processing, heat treat- ment, testing, and finishing operations must all be closely controlled at each step to ensure that products have the required characteristics [11-14] . RECYCLING AND ENVIRONMENTAL CONCERNS Due to the high buy-to-fly ratio (as high as 9:1), recycling of titanium (revert) is an economic necessity. Recy- cling companies come into play at both the beginning and end of the process. Scrap is readily available at high man- ufacturing rates, which is purchased by the recycler, processed, and sold to an ingot producer. Until the 1980s, use of scrap was limited because it was difficult to re- move impurities. High density inclu- sions, such as the broken tungsten-rich tool bits from aerospace manufactur- ing production had to be removed from turnings to preclude being melted into the ingot, which could lead to defects resulting in failure of aerospace engine parts. With the removal of impurities, titanium turnings became an essential component of premium quality ingot. TABLE 1 — CHEMICAL COMPOSITION AND SPECIFICATIONS FOR COMMON TI ALLOYS Nominal composition, wt% Common name UNS No. Aerospace Materials Specification (AMS) ASTM Standard B265 U.S. Military Specification Alpha ( a ) alloys 99.5 Ti Ti R50250 4591E Grade 1 Mil-T-9046J 99.2 Ti Ti R50400 4902E Grade 2 Mil-T-9046J 99.1 Ti Ti R50550 4900J Grade 3 Mil-T-9046J 99.0 Ti Ti R50700 4901L Grade 4, 7, and 11 Mil-T-9046J 99.8 Ti Ti-0.2 Pd R52400, R52250 - - - Ti-5Al-2.5Sn Ti-5-2.5 R54520 4926H Grade 6 Mil-T-9047J Ti-5.8Al-4Sn-3.5Zr-0.7Nb-0.5Mo-0.35Si IMI 834 - - - - Ti-8Al-1Mo-1V Ti-811 R54810 4972C - Mil-T-9047G Ti-6Al-2.7Sn-4Zr-0.4Mo-0.45Si TiMetal 1100 - - - - Alpha-beta ( α - β ) alloys Ti-3Al-2.5V Ti-3-2.5 R56320 4943D Grade 9 Mil-T-9047G Ti-6Al-2Sn-4Zr-2Mo-0.1Si Ti-6242S R54620 4976C - Mil-T-9047G Ti-6Al-4V Ti-6-4 R56400 4911F Grade 5 Mil-T-9046G Ti-4Al-4Mo-2Sn-0.5Si Ti-550 - - - - Ti-6Al-6V-2Sn Ti-662 R56620 4918F - Mil-T-9046J Ti-6Al-2Sn-2Zr-2Mo-2Cr-0.1Si Ti-6-2222S - - - - Ti-6Al-2Sn-4Zr-6Mo-2Cr-0.1Si Ti-6246 R56260 4981B - - Ti-4.5Al-3V-2Mo-2Fe SP700 4899 - - - Ti-5Al-2Sn-2Zr-4Mo-4Cr Ti-17 R58650 4955 - - Beta ( β ) alloys Ti-10V-2Fe-3Al Ti-10-2-3 - 4984 - - Ti-15V-3Cr-3Al-3Sn Ti-15-3 - 4914 - - Ti-3Al-8V-6Cr-4Mo-4Zr Beta C R58640 4957 Grade 19 Mil-T-9046J Ti-3Al-2.8Nb-15Mo-0.2Si TiMetal21S R58210 - - - Intermetallics Ti 3 Al Alpha 2 - - - - TiAl Gamma - - - -
Made with FlippingBook
RkJQdWJsaXNoZXIy MjA4MTAy