April_AMP_Digital

A D V A N C E D M A T E R I A L S & P R O C E S S E S | A P R I L 2 0 1 8 22 Several environmental concerns associated with titanium production include waste disposal, air quality, fire hazards, and others. Residuals contain- ing heavy metals in the chlorination of rutile to TiCl 4 present a disposal prob- lem. The potential for leaking Cl 2 and TiCl 4 also exists. Transport of TiCl 4 to sponge producers that have no TiCl 4 production is done by rail, which is a concern, as is the handling of Cl 2 , which is generated but not consumed. Sponge production is leached or washed, and there is a concern with effluent from these operations. Pickling is intrinsic to most tita- nium mill operations, especially those that make flat products. Acid baths build up dissolved metal ion content, so disposal of the liquid is a significant problem especially because it contains fluorine ions. The industry is evaluating ways to minimize or eliminate hydroflu- oric acid pickling where possible. Further, there is always the poten- tial for titanium fires in the sponge plant and chip plant as well as in pow- der metallurgy operations. This is more of a safety issue than an environmen- tal problem. APPLICATIONS Over the past 40 years, titanium use in military, commercial, and con- sumer applications has continued to grow, depending in part on fabricabil- ity and cost [10] . Product requirements for titanium alloys in each market seg- ment are based on specific needs of the particular application. For example, jet engine requirements focus primarily on high-temperature tensile and creep strength, as well as thermal stabili- ty at elevated temperatures. Second- tier property considerations include fa- tigue strength and fracture toughness. Airframe applications require high ten- sile strength combined with good fa- tigue strength and fracture toughness. Ease of component fabrication is also an important consideration. Industri- al applications demand good corro- sion resistance in a variety of media as a prime consideration as well as ade- quate strength, fabricability, and com- petitive cost relative to other types of corrosion-resistant materials. The high cost of titanium alloy often limits its application. Thus, a lot of research is aimed at reducing component cost while maintaining acceptable mechani- cal property levels; approaches include near-net-shape techniques and lower cost alloy formulation. The use of titanium in terrestrial military vehicles leads to high-perfor- mance attack systems that are strong, lightweight, fast, and readily deploy- able with cost penalties being resolved by single melt and near-net-shape fab- rication. However, the aerospace in- dustry dominates the use of titanium in engines and airframes. Fan and com- pressor blades, discs, and hubs made of titanium account for about 30% of the weight of a gas turbine engine. Titanium offers high strength-to-weight ratio, strength at moderate tempera- tures, and good resistance to creep and fatigue. In the airframe, titani- um brings about weight reduction in highly stressed parts. According to the International Titanium Association, en- gines account for about 42% of U.S. ti- tanium demand and 37% in Europe [10] . Figure 3 shows the power unit for the F-35 Lightning, which contains a sub- stantial amount of titanium. The Boe- ing 777 uses 13,000 lb forging weight of Ti-10V-2Fe-3Al in the landing gear. The Boeing 787 requires at least 120 tons forging weight of titanium per aircraft including the engines. U.S. Navy ships CVN 77 and CVN 78 use 38 tons of Ti-6Al-4V alloy per ship for mainmast platforms (Fig. 4) in the Fig. 3 — Current and potential applications of titanium in passenger cars. Fig. 4— The LockheedMartin F-35 Lightning II engine contains a substantial amount of titanium.

RkJQdWJsaXNoZXIy MjA4MTAy