April_AMP_Digital
A D V A N C E D M A T E R I A L S & P R O C E S S E S | A P R I L 2 0 1 8 20 processes, allowing use of the product in the current value chain. However, the powder is better used in direct non- melt consolidation to final end product, eliminating the need to process sponge, thereby reducing supply chain cycle time, energy consumption, manufac- turing costs, and environmental impact. An advantage of the process is its ability to produce a range of alloys (including Ti-6Al-4V) as a high-quality homoge- neous powder suitable for many appli- cations. The Lockport facility provides limited quantities of materials nec- essary to successfully complete sol- id-state consolidation development activities. ITP also broke ground on a 4 million lb/yr facility in Ottawa, Ill., to produce CP Ti and Ti-6Al-4V alloy pow- der. Independent research shows the use of low-grade TiCl 4 leads to higher part density due to the difference in sin- tering behavior that affects the entrap- ment of volatiles within the sintered body. As of late 2017, the full-scale facil- ity had not yet entered production. Materials and Electrochemical Re- search Corp. (MER) and DuPont are de- veloping an electrolytic powder process that uses a composite anode of TiO 2 (re- ducing agent) and an electrolyte mixed with fused halides [1] ; Ti is deposited at the cathode. Ti production is project- ed at significantly lower cost than the Kroll process. Advanced Materials (ADMA) Prod- ucts, Hudson, Ohio, is developing a powder process in which sponge titani- um is cooled in a hydrogen atmosphere rather than conventional inert gas. The hydrogenated sponge is easily crushed and can be compacted in the hydro- genated condition to a higher density than that of conventional low-hydro- gen sponge. Reportedly low levels of remnant chloride content of the hydro- genated sponge helps to avoid porosity and enhance weldability. Fang et al. [6] studied the use of hy- drogen-assisted reduction of TiO 2 with magnesium and production of low-cost spherical meltless Ti powder. ECONOMIC ASPECTS Figure 2 shows the uses of Ti raw material. U.S. imports for consump- tion of titanium pigment were nearly 290,000metric tons in 2006. U.S. exports of titanium by class (scrap, unwrought, wrought, ferrotitanium and ferrosilicon titanium, ores and concentrates, and pigment) were 581,000 metric tons in 2006. Regarding titanium pigment ship- ments, roughly 57% were used in paint, 26% in plastics and rubber, 12% in pa- per, and 4% in other applications [9] . In 2007, titanium sponge pro- ducers in the U.S. included ATI, Titani- um Metals Corp. (Timet), and The Alta Group (part of Honeywell Electronic Materials Inc.). ATI’s sponge plant ca- pacity increased to 7260 metric tons/yr, and the company began construction of a new premium-grade sponge plant in Rowley, Utah. ATI began construction of a sponge plant in Hamilton, Miss., to be operational by 2010. Timet increased its sponge capacity and brought a new EB furnace and several VAR furnaces online in 2008. However, the economic downturn later that year led to a severe slowing of plant construction across the industry. ATI idled its Albany, Ore., sponge plant (Wah Chang unit) and de- layed bringing the Rowley facility online until late 2009. Prior to the downturn, production of titanium metal products rose to record levels; U.S. ingot produc- tion reached 59,200metric tons, an 11% increase over 2006 [10] . Before 1970, more than 90% of ti- tanium products were used in aero- space applications, which fell to about 70-80% by 1982. Military use also de- clined through the late 1990s [10] . How- ever, industrial demand for titanium continued to increase through the late 1990s and into the new millenni- um. While the destruction of the World Trade Center in New York City on Sep- tember 11, 2001, had amarked negative effect on commercial aerospace, Boe- ing and Airbus began to receive orders for their new planes, the 787 Dreamlin- er and A380, respectively, both of which contain between 130 and 150 tons of titanium components per unit. Also, production of the U.S. Air Force F-22 Raptor began in 2003. Simultaneous- ly, there was a price surge in titanium, more than doubling between 2003 and 2006. The recession beginning in 2008 reversed the cycle with cancellations outnumbering orders of new planes. Production of the F-22 came to an end, replaced by production of the F-35 Lightning II. The breakup of the former Soviet Union drastically reduced internal con- sumption of titanium, leaving a large volume available for export. Through- out the 1990s, VSMPO-AVISMA upgrad- ed its quality standards so its products could be used in aerospace applica- tions, completing its transformation by 2000. By 2009, the company was ex- porting 70% of its products, with the remainder supplied to the domestic market. GRADE, SPECIFICATIONS, QUALITY CONTROL Commercially important titani- um grades and pertinent specifications are shown in Table 1. In addition, every Fig. 2 — U.S. titanium rawmaterial use [7,8] .
Made with FlippingBook
RkJQdWJsaXNoZXIy MjA4MTAy