August_EDFA_Digital

edfas.org 25 ELECTRONIC DEVICE FAILURE ANALYSIS | VOLUME 20 NO. 3 contrast represents a shi¨ in current flow through the con- ductor. Typically, an abrupt contrast change is observed on “hard” open failures and a gradual contrast intensity change is observed on marginal or “so¨” open failures. CURRENT IMAGING Another complementary method for measuring current flow inside a sample is current imaging (CI). This method employs a probe tip that is brought into contact with the sample. With the tip gently touching the surface, it is scanned over the area of interest in a line-by-line fashion. The tip can be biased to a given voltage and the current flow to bulk is recorded for each scan point. Once the tip is in contact with the sample, the electron beam can be blanked, thus minimizing contamination of the sample surface as well as the probe tips. The obtained data is recorded and used to generate a map of current flow in the scanned area. As semiconductor samples are flat by nature and the scanned area is comparatively small, the experimental setup can be greatly simplified by foregoing the use of AFM-based methods. The simplicity of this approach allows the operator to choose any of the available probe tips—up to eight using the Prober Shuttle—to act as the scanning tip. Additionally, any of the available probe tips or the sample bulk can be configured either as voltage source or current sink. It is also possible to scan the bulk under a stationary tip. This allows the operator to specifi- cally search for certain artifacts or faults. For example, a leaky gate will produce a current response during the CI sweep if the sample bulk is configured as the current sink, where healthy transistor gates will not show a response on the current map. A beneficial side eƒect to the sweeping motion used in the CI technique is that this gentle scrubbing action can be used to remove surface contaminants from the sample, thus providing a clean surface for subsequent probing experiments. INSTRUMENTATION The experiments described in this article were per- formed using a Kleindiek Nanotechnik Prober Shuttle. This platform is available in two sizes: 100 mm diameter for up to four probes and 140mmdiameter for up to eight probes. Probes are positioned using piezomotors for high stability and positioning accuracy. The Prober Shuttle’s low profile allows for inserting the platform via a suitable load lock aswell as imaging at very lowworking distances. The latter is especially important when using low accel- eration voltages. The probing system can be enhanced with an array of measurement tools and control so¨ware. Notably, the EBIC/RCI amplifier described abovewas used on the experiments discussed here. Additional modules, such as the CI option, are described below. FAILURE ANALYSIS CASE STUDIES CASE #1: LOCATING RESISTOR CHAIN DEFECTS The device under test (DUT) in this case consisted of a continuous contact chain between silicided N-active islands and the metal 1 layer manufactured in 28 nm technology. In the first case, this chain exhibited a high ohmic link failure that was found during in-fab electrical testing. It exhibited increased resistance of the entire resis- tor chain. The EBAC techniquewas employed by placing a probe tip at each end of the resistor chain, while routing one probe tip to ground and the other to the EBAC ampli- fier. While the electron beam is swept across the sample surface, the resulting EBAC signal is displayed on the microscope screen, revealing the location of a high-ohmic link in the via chain (Fig. 2). A subsequent site-specific Fig. 1 EBIC signal generation. Fig. 2 EBAC result on resistor chain. The yellow circle indicates the fault’s location.

RkJQdWJsaXNoZXIy MjA4MTAy