August_EDFA_Digital
edfas.org ELECTRONIC DEVICE FAILURE ANALYSIS | VOLUME 20 NO. 3 24 LOCATING FAILURES IN CURRENT DEVICE NODES: EBIC/EBAC, CURRENT IMAGING AND NANOPROBING Stephan Kleindiek 1 , Rosalinda M. Ring 2 *, Klaus Schock 1 , Andreas Rummel 1 , Michael Zschornack 3 , Pascal Limbecker 3 , Andreas Meyer 3 , Randy Newkirk 2 , Kevin Davidson 2 , Matthias Kemmler 1 1 Kleindiek Nanotechnik, Reutlingen, Germany 2 GlobalFoundries, Malta, N.Y. 3 GlobalFoundries, Dresden, Germany EDFAAO (2018) 3:24-33 1537-0755/$19.00 ©ASM International ® INTRODUCTION The ever-decreasing line widths in modern semicon- ductor products, required for delivering higher perfor- mance devices that consume less power, can create new challenges for process ramps and yield management. Electrical fault isolation (EFI) is an important tool for locating faults. Once the general region of a fault has been identified, nanoprobing is o¨en used to precisely locate the fault. Next, further analysis of the fault’s root cause is performed, e.g., by preparing a site-specific transmission electron microscopy (TEM) section. As semiconductor nodes get smaller and smaller, there is an increasedneed tomove a large portion of EFI to scan- ning electron microscopes (SEMs) or combined focused ion beam (SEM/FIB) tools. Prior to moving into SEM or FIB/SEM, samples are typically processed on other test platforms using an array of analysismethods to locate the region of interest (ROI) on the sample—one suchmethod is optical beam induced resistance change (OBIRCH). The scanning electronbeam ismainly used to generate images of the sample surface—for device inspection or to assist in landing probe tips for electrical measurements. The FIB can be used to remove or deposit material. This can be useful for preparing TEM slices for further analysis or for modifying circuits in-situ. EBIC AND EBAC When imaging the sample, the electron beam will penetrate the sample surface where it can interact with the conducting lines in the device layers. When using probe tips strategically placed on contacts on the sample surface, combinedwith a highly sensitive amplifier, these induced currents can be recorded and visualized by feeding the recorded current back to the microscope. In thismanner, an image is generated of the currents flowing throughout the conducting lines that the probe tip is in contact with. The electron beam induced current (EBIC) imaging technique [1,2] reveals the location of P-N junctions and the quantitative amount of current flowing to and from them. EBIC imagery is generated by reading a low current signal from the sample—thus a well shielded, low-noise lead is required from the probe tip (that is in contact with the sample) all the way to the EBIC amplifier. Using this type of signal lead, the current induced by the electron beam can be recorded, amplified, converted to a voltage, and fed back into the SEM where it is registered as an auxiliary detector signal. Thus, the EBIC signal is gener- atedwithin themicroscope’s control so¨ware and can be superimposed on the secondary electron (SE) image for easy identification of the ROI. A schematic of EBIC image generation is shown in Fig. 1. A similar approach, known as electron beamabsorbed current (EBAC) or resistive contrast imaging (RCI), [3] can be used to reveal conductive areas that are buried in the device layers while contacted to the probe tip via a pad on the sample surface. If the current path exhibits an “open” defect, the resulting EBAC image shows an abrupt change in contrast. In the case of a “resistive open” defect, a gradual contrast change is observed. This change in *Now with Lam Research.
Made with FlippingBook
RkJQdWJsaXNoZXIy MjA4MTAy