February_EDFA_Digital
edfas.org 1 7 ELECTRONIC DEVICE FAILURE ANALYSIS | VOLUME 20 NO. 1 a monograin-affected transistor. It allowed the develop- ment of a dedicated simulation program with an inte- grated circuit emphasis (SPICE) model that was used to reproduce, at the design level, observations (signal slope/ delay) acquired with LVP. CONTAINMENT AND CORRECTIVE ACTIONS The monograin issue is closely linked to both process and design factors. Several containments have been applied at the process level, such as doping of transis- tors, control of grain growth, optimization of the poly- silicon height, and so on. At the design level, because the monograin stronglydepends on scaling, critical transistors have been redesigned to avoidorminimize the occurrence and impact of gate monograin issues. High-speed clock- drivengateswith small poly areas havebeen replacedwith a longer poly shape, review of some regular poly layout, automatic detection algorithms included in the verifica- tion flow, margin simulations using the dedicated SPICE model developed for themonograin issue, and soon. All of these “robustization” actions concerning the monograin issue affecting just a few parts per million of transistors led to a significant gain in yield and better margins in maximum frequencies. CONCLUSION Finding the monograin failure mechanism required a high number of failing parts and was time-consuming. Even though failure localization was quite “classical” in the failure analysis flowusing SDL and LVP, the difficulties occurred at parametric verification during nanoprob- ing and TEM analysis. Electrical measurements showed proper transistors, and physical observation in the TEM showed a proper morphological device. It was difficult to be convinced that the located failing transistor was the correct one until the monograin failure hypothesis was tested using TEM observation along the gate instead of across the gate of the transistor. Failure analysis of the monograin required the use of techniques frommaterial crystallography analysis, such as nanobeam diffraction with automatic crystal orientation/phase mapping, to prove the single orientation of the grain compounding the gate. With the support of TCAD and design, test, and process teams, the root cause and failure mechanism has been clearly explained, leading to the production of dedicated physical and electrical simulation tools to resolve the failure mode. Transistor gates have now been “robustized” by design and optimized in process to limit the effect of this specific defect that impacts integrated circuits of nanoscale technology nodes. REFERENCES 1. B. Fultz and J.M. Howe: Transmission Electron Microscopy and Diffractometry of Materials, Springer Science and Business Media, 2012. 2. M.R. Bruce, V.J. Bruce, D.H. Eppes, J.Wilcox, E.I. Cole, P. Tangyunyong, C.F. Hawkins, and R. Ring: “Soft Defect Localization (SDL) in Integrated Circuits Using Laser Scanning Microscopy,” Lasers and Electro-Optics Society (LEOS) 2003, Vol. 2, The 16th Annual Meeting of the IEEE, Oct. 2003, pp. 662-63, ieeexplore.ieee.org/abstract/ document/1252974. 3. S. Kolachina: “Introduction to Laser Voltage Probing (LVP) of IntegratedCircuits,” Microelectronics Failure Analysis, DeskReference, 6th ed., ASM International, 2011, pp. 349-53, asminternational.org/ web/edfas/search/-/journal_content/56/10192/MEFA2011P349/ BOOK-ARTICLE. 4. L.A. Bendersky and F.W. Gayle: “Electron Diffraction Using Transmission ElectronMicroscopy,” J. Res. Natl. Inst. Stand. Technol., 2001, 106 , pp. 997-1012. 5. A. Kobler, A. Kashiwar, H. Hahn, and C. Kübel: “Combination of In Situ Straining and ACOMTEM: A Novel Method for Analysis of Plastic Deformation of NanocrystallineMetals,” Ultramicroscopy, 2013, 128 , pp. 68-81, doi.org/10.1016/j.ultramic.2012.12.019. 6. E.F. Rauch andM. Véron: “Automated Crystal Orientation and Phase Mapping inTEM,” Mater. Charact., 2014, 98 , pp. 1-9, doi.org/10.1016/j. matchar.2014.08.010. 7. A. Valery: “Microtexture Characterization by Automated Crystal Orientation Mapping in TEM for the Development of Advanced Technologies in Microelectronics,” SiMap, I-MEP2, Grenoble INP University, 2017. 8. R.R. Keller and R.H. Geiss: “Transmission EBSD from10 nmDomains in a Scanning Electron Microscope,” J. Microsc., 2011, 245 (3), pp. 245-51, doi.org/10.1111/j.1365-2818.2011.03566.x. ABOUT THE AUTHORS Thierry Parrassin obtained a Master’s degree in microelectronics from the Institut National Polytechnique de Grenoble in 2010. He joined STMicroelectronics as a failure analysis technician in 1999, where he is currently a failure analysis engineer. His mission is to support both manufacturing and research and development activities on site through basic and advanced failure analysis. Thierry is a specialist in test engineering, design debug, defect-localization techniques, photoemission (emission microscopy), laser stimulation mapping (OBIRCH, TIVA, laser-assisted device alteration, soft defect localization, fault injection mapping), laser mapping (laser voltage imaging, variation mapping, thermal frequency imaging, second-harmonic degradation mapping), and contactless
Made with FlippingBook
RkJQdWJsaXNoZXIy MjA4MTAy