April_AMP_Digital

A D V A N C E D M A T E R I A L S & P R O C E S S E S | A P R I L 2 0 1 8 3 1 directional scratches were imparted in the sample surface during polishing (Fig. 3a). As a result, the poor quality Euler map obtained from this sample should be expected (Fig. 3b). ION MILLING As a final stage in sample prepara- tion, ion milling is an option that elimi- nates much of the variation inherent to hand polishing and ensures amore con- sistent and higher quality surface finish. With ion milling, the sample is polished as usual down to a one-micron partic- ulate slurry. It is then bombarded with argon ions at an angle of 20° to 50° at an accelerating voltage of 1−30 kV. The ion bombardment removes material from the surface by sputtering. Systematically lowering the accel- erating voltage reduces both the rate of material removal and the depth of ion penetration into the material, which in turn systematically reduces the dam- age layer imparted on the surface during the removal process. A final pol- ishing step between 1 and 3 kV results in virtually no surface damage. The effectiveness of broad ion milling for EBSD sample preparation is demonstrated in Fig. 4. Here, an alumi- num sample was prepared as described above with the exception that only the left-hand side of the sample was pol- ished by ion milling. In the electron im- age, the grain structure is clear on the left with a general reduction in quality moving to the right with only a few grains visible (Fig. 4a). In the corre- sponding Euler map, the grains with identified crystal orientation are clear and unambiguous on the left (Fig. 4b). The only exception is a deep scratch angled diagonally through the sample. Moving to the right, the indexing quality degrades so that less than half of the grains are properly identified with EBSD. This ion milling technique can be applied to a cast iron sample subject to graphitic corrosion within a chlo- rinated environment. Cast iron lacks the nickel or chrome additives pres- ent in stainless steel and is therefore at risk of corrosion. An optical image of a corroded section is shown in Fig. 5a. The sample is mounted in epoxy, pol- ished to one-micron grit, and then ion milled with a monatomic argon beam for 30 minutes and finally at 3 kV for 10 minutes with an Ar + cluster ion source. The electron image demonstrates the grain structure with dark tendrils en- croaching throughout the sample (Fig. 5b). Energy dispersive spectrosco- py and wavelength dispersive spectros- copy (EDS/WDS) confirm the presence of chlorine and a higher level of carbon in these dark, tendril regions with no de- tected chlorine and lower levels of car- bon throughout the remainder of the sample. An overlay of the Euler maps from EBSD analysis on the electron im- age confirms the nature of the corro- sion (Fig. 5c). The ferritic grain structure expected from uncorroded cast iron is demonstrated, and the dark, tendril re- gions yield no diffraction patterns, in- dicating an amorphous structure as expected from this type of corrosion. SUMMARY EBSD combined with EDS and electron imaging yields a wealth of rich information regarding the material mi- crostructure. Because EBSD is a sur- face-sensitive technique, preparing the sample surface so that it is smooth and free of defects is crucial to successful analysis. Traditional hand polishing can achieve high-quality results, although the technique is prone to variation and Fig. 3 — (a) Scratches imparted into sample surface during polishing; (b) poor quality Euler map obtained from sample. (b) (a) (b) (a) Fig. 4 — (a) Left-hand side of image polished by ion milling is clear; grain structure image quality degrades from left to right; (b) corresponding Euler map shows clear grains on left with degrad- ing indexing quality to the right.

RkJQdWJsaXNoZXIy MjA4MTAy