August_EDFA_Digital

edfas.org ELECTRONIC DEVICE FAILURE ANALYSIS | VOLUME 20 NO. 3 32 metal 1 contact (CA) chain to islands of active (RX) regions with dummy parallel PC lines. The split lot wafer showed an elevated number of so¨ failures at 12 o’clock. RCI analysis at 2 kV/1.6 nA localized the defect to two adjacent contacts. The FIB cross-sections and advancedTEManaly- sis showed evidence of the presence of a particle between the contact and active (CA/RX) layers (Figs. 19, 20). The particle appeared to have blocked the CA etch resulting in an unlanded CA, which resulted in the observed electrical “open” failure. SUMMARY Advances in integrated circuit (IC) technology have made failure site localization extremely challenging. Muchwork has been done to eƒectively and rapidly detect defects on ICs during fabrication. The nanoprober based current imaging system pro- vides a number of advantages for SEM (or FIB/SEM) based failure analysis. Among these are easy navigation to the region of interest (using the SEM), fast and contamination- free imaging of the contacts (using CI), and the possibility of performing nanoscale probing in situ without moving to a separate tool. When combined with EBIC/EBAC/RCI, the nanoprober is equipped with additional capabilities for elucidating the root cause of common failures. This work demonstrates that RCI is a valuable defect localization technique for “soft” or “marginal” open failures aƒecting the full range of process modules with defect sizes in the 20 to 50 nm range or on defects buried beneath multiple layers of metals. REFERENCES 1. W. Ehrenberg, C.S. Lang, and R. West: “The Electron Voltaic Eƒect,” Proc. Phys. Soc., 1951, A 64, p. 424. 2. T.E. Everhart, O.C. Wells, and R.K. Matta: “Evaluation of Passivated Integrated Circuits Using the Scanning Electron Microscope,” Electrochemical Society, electronics division, 1963, 12 (2), p. 2-4. 3. E.L. Cole Jr.: “Resistive Contrast Imaging applied to Multilevel Interconnection Failure Analysis,” IEEE 6th VLSI Multilevel Interconnection Conference, 1989, p. 176. 4. R. Rosenkranz: “Failure Localizationwith Active and Passive Voltage Contrast in FIB and SEM,” J Mater Sci Mater El, 2011, 22 (10), p. 1523. 5. R. Rosenkranz, S. Doering, W. Werner, and L. Bartholomaeus: “Active Voltage Contrast for Failure Localization in Test Structures,” Proc. Int. Symp. Test. Fail. Anal. (ISTFA), 2006, p. 316-320. Fig. 19 High-angle annular dark-field scanning transmission electron microscopy (HAADF STEM) image of the defect site highlighting the unlanded contact. Fig. 20 Energy dispersive x-ray (EDX) map of the area shown in Fig. 19 reveals the presence of a particle between theRX and the CA layers. The particle appears tohave blocked the CA etch, resulting in unlanded CAs. ABOUT THE AUTHORS Stephan Kleindiek studied physics inMarburg and Tübingen, Germany. A¨er a six-month visit to IBM’s T.J. Watson Research Center in Yorktown Heights, N.Y., in 1994, he finished his Ph.D. in 1996 and founded Kleindiek Nanotechnik in 1997, where he now serves as CEO. He invented the Nanomotor and subsequent rotational motors, which are the foundation for his company's products. Rose M. Ring has a master’s in chemistry from the University of New Hampshire. She is a failure analyst, inventor, and FA lab manager. She joined GlobalFoundries in 2011 and provided extensive FA and material characteriza- tion support for the 14 nm development teams. She is currently a microscopist at Lam Research supporting advanced fabrication process development. Klaus Schock studied physics at the Eberhard-Karls-Universität in Tübingen focusing on elec- tron lithography and electronics. He works on electronic, mechanical, and so¨ware development and applied research in the field of electrical probing, sample preparation, and manipulation at Kleindiek Nanotechnik.

RkJQdWJsaXNoZXIy MjA4MTAy