May_EDFA_Digital

edfas.org 31 ELECTRONIC DEVICE FAILURE ANALYSIS | VOLUME 20 NO. 2 (e.g., FIB deposition) needed. [8] The TEM image in Fig. 5b shows a gate structure that was FIB milled in a backside orientation after beingmanipulated to a slotted half-grid. Note the absence of curtaining artifacts due to the fast and easy geometry achieved. OPTIMIZING VAN DER WAALS FORCES As previously mentioned, van der Waals forces are directly proportional to the surface area of the features touching. Thus, the probe surface area can be shaped to create large flat solid surfaces, thereby increasing the VDW forces by a factor of two to 10 or more. [9] The probe angle and the FIB specimen’s orientation relative to the probe can be adjusted to match the orientation of the beveled probe surface. Elliptical flat surfaces or polygonal-shaped probe surfaces similar to that shown in Fig. 6 can be used to lift out the specimen and optimize the manipulation techniques to slotted half-grids. [9] VACUUM-ASSISTED EXLO FOR PLAN- VIEW SPECIMEN PREPARATION In addition to using solid cylindrical or shaped probes for EXLO via VDW forces, it is also possible to supplement VDW forces by using beveled hollowglass tubes combined with vacuum suction. [6] Plan-view specimen preparation via EXLO has previously been reported. [13] Recently, the application of vacuum-assisted EXLO specifically for FIB preparation of plan-view specimens has been em- ployed. [14] Vacuum-assisted EXLO methods aid in track- ing the precise direction and orientation of the specimen during the lift out and manipulation steps. A schematic diagram of the process is shown in Fig. 7. First, the FIB is used to completely mill free a triangular prism shape from a region of interest as in Fig. 7a. Then the sample is lifted out via EXLO, using a beveled hollowprobe attached to a vacuum pump to provide suction through the probe (Fig. 7a). In this orientation, the probe bevel and attack angle are orientated parallel to the lift out surface. After the specimen is secured to the probe, the probe is raised and rotated 180 o (Fig. 7b). The probe is lowered and the vacuum is turned off just prior to manipulating the lift out specimen to the grid. The probe slides through the slot, allowing the specimen surface to rest on the slotted half-grid (Fig.7c). Finally, the grid with the specimen is returned to the FIB for milling on the plane of interest for plan-view analysis. S/TEM results from various materials will be presented in a future publication. [14] SUMMARY AND CONCLUSIONS This article presents recent advances in EXLOprocess- es. In summary, the EXLO process is fast, easy, reproduc- ible, and cost effective for high throughput FIB specimen preparation for conventional and high-resolution S/TEM. In addition, site-specific FIB lift out specimens can be easilymanipulated via EXLO for other site-specificmateri- als characterization methods. New EXLO methods allow for additional flexibility of techniques, eliminating the need for a thin film support, allowing for fast and easy backside thinning, reducing curtaining artifacts, and adding vacuum-assisted lift out for plan-view specimen preparation and more. ACKNOWLEDGMENTS EXpressLO grids and methods are covered under U.S. Patents 8,740,209 and 8,789,826. Optimization of van der Waals forces using beveled solidprobes is patent pending. (a) (b) (c) (a) (b) (c) Fig. 6 Schematic diagram of solid probe flat tip shapes (a) elliptical and (b,c) polygonal surfaces. Fig. 7 Schematic diagram of process steps for plan-view vacuum-assisted lift out including (a) lift out (b) rotation, and (c) manipulation to a slotted half-grid.

RkJQdWJsaXNoZXIy MjA4MTAy