edfas.org 7 ELECTRONIC DEVICE FAILURE ANALYSIS | VOLUME 20 NO. 1 Fig. 8 Contact failure caused by metal wear. Arcing occurs and burns the contact surfaces. Fig. 9 If a particle blocks the contact, and if the distance between the contact surfaces is not too large, arcing can occur (basic rule: 1 V/µm in air). The arc burns at the point, which represents the closest distance between the contacts. If the particle (see arrows for the mark) is located somewhat away, it will not burn or sink into the molten contact surface. Material can be transported if direct current is involved, forming a tip and a hole. Fig. 10 The black regions in the scanning electron microscopy image of the contact point of a failed relay contact indicate nonconductive layers. They consist of silicon dioxide, shown in the energy-dispersive x-ray spectrograph. The SiO 2 is produced in the electrical arc from silicone vapor and condenses in the contact region.