February_EDFA_Digital
edfas.org 23 ELECTRONIC DEVICE FAILURE ANALYSIS | VOLUME 20 NO. 1 previous polishing step. With the final polishing step, the goal was to have no polishing damage (neither scratches nor crystal deformation) left in the tin as a result of speci- men preparation. The specimens were imaged using optical metallog- raphy in both bright-field imaging and polarized light, with the polarizers nearly crossed (cross polarizer, or XP, imaging). The XP imaging contrast in tin arose from the birefringent properties of tin, leading to different colors for different crystal orientations of tin under XP ima- ging. [31] Selected specimens were imaged using SEM. Images were taken using backscatter electron (BSE) imaging. InBSE compositionmode images, contrast is pro- portional to the average atomic number of the material. MEASUREMENTS OF SHEAR STRENGTH The shear strength tests were conducted using a DAGE Series 4000 Plus bond tester. The shear loading speed was 700 µm/s (with a maximum test load of 400 g) (Fig. 4), in accordance with the JEDEC JESD22- B117A standard. [32,33] Measurements done at room tem- perature were repeated on multiple nominally identical samples. The dependence of shear strength on system parameters (e.g., solder composition, size, andaging time) and on shear strengthmeasurement parameters, such as shear height, was examined. Shear test was performed on both copper pillar and solder cap. ACCELERATED THERMAL CYCLING TEST An ATC test was performed at Universal Instruments Corporation. A − 40/125 °C ATC test was used with 15 min dwell times at the temperature extremes and 9 °C/min transition rates between the extremes, consistent with IPC-9701 criteria. [34] A solder joint failurewas definedwhen the resistance of the joint exceeded 900 Ω . Generally, after failure was detected, samples were removed from the chamber for microstructural characterization. RESULTS The effect of composition and aging on themicrostruc- ture and shear strength of copper pillar solder joints was examined. Themicrostructure of the solder joint was eval- uated in the as-fabricated configuration and after aging. Varying the solder composition or the thermal history of SnAg or SnAgCu solder joints affects their microstructure and their mechanical response. [1-6] The number, size, and arrangement of Ag 3 Sn precipitates affect the mechanical response of Sn-Ag-Cu near-eutectic solder joints and their reliability. [1–8] A large number of fine Ag 3 Sn precipitates (Fig. 5) would be expected to be much stronger than one Fig. 4 Schematics of low-speed shear test. Shear test was performed on both (a) solder cap and (b) copper pillar. Source: Ref 33 (b) (a) with a few large Ag 3 Sn precipitates (Fig. 6, micrographs for aged samples). A number of different thermal history parameters influence theSn-Ag-Cumicrostructure, includ- ing aging time. A fine Ag 3 Sn precipitate morphology in Sn-Ag-Cu solder (such as that of Fig. 5) will coarsen over time, particularly at elevated temperatures, and the mechanical properties of the solder would be expected to change. These effects were examined for copper pillar solder joints before and after aging. The effect of silver concentrationon themicrostructure of copper pillar/SnAg solder joints is illustrated in Fig. 5. A number of Ag 3 Sn precipitates are seen in all of the joints containing silver, even for the solder joint with solder containing 0.9% Ag. The spacing between precipitates ranged from 0.1 µm to approximately 2 µm, with more submicron spacings for the solder joint containing 2.4%Ag
Made with FlippingBook
RkJQdWJsaXNoZXIy MjA4MTAy