February_EDFA_Digital
edfas.org 15 ELECTRONIC DEVICE FAILURE ANALYSIS | VOLUME 20 NO. 1 identified as the failing location. After deprocessing of several failing dice down to the contact level, the static parametric characteristics of that PMOS are measured and compared with a good reference transistor in nano- probing. The measurements show a perfectly working transistor. This result proves that the defect has pure dynamic and transient effects. Observing the defect with TEM was very costly in terms of used candidates until a good orientation was finally found for lamella extraction: lengthwise of the polysilicon gate, along the width of the transistor. Nevertheless, the defect is still invisible in clas- sical TEMor scanning-TEM (STEM). Figures 5(b) and (c) do not show any difference between the failing transistor and a reference one. Before concluding that the failing transistor has no anomalies, TEM dark-field imaging (Fig. 5d) provides qualitative results on the microstructure: one main orientation difference is observed through the polytungsten of the failing PMOS. Due to artifacts in the diffraction contrast leading to shadow areas, dark-field imaging always leaves some doubts in the interpretation of the polysilicon gate grain orientation. The nanobeam electron diffraction (NBD) technique [4] is used for quantitative measurement of the grain orientation, providing more reliable results. The principle of NBD is rather simple. As shown in Fig. 6, a parallel electron beam with small diameter is formed in the TEM and scanned across the sample. The resulting diffraction patterns are recorded and analyzed for each location with a high-speed, high-resolution charge-coupled device (CCD) camera. Local orientation and phase information on polycrystalline materials can be extracted from diffraction spot positions. Approximately 50 NBD patterns are acquired over a line profile in the polysilicon of the reference and failing PMOS transistor using an electron probe size of 5 nm. Figure 7 shows different diffraction patterns along the gate, revealing multiple grains through the polysilicon. On the failing PMOS, the same lattice plane is systemati- cally present through the polysilicon; onemain diffraction pattern is observed, revealing only one grain in the gate of this transistor. The synchronization between e-beam scanning and the fast-acquisition CCD camera (up to 200 patterns/ second) with postprocessing computation of the data allows the transposition of line profiles into automatic crystal orientation/phasemapping (ACOM). [5-7] It produces an orientationmap similar to electron backscatter diffrac- tion [8] in scanningelectronmicroscopybasedon the collec- tion of electron diffraction patterns and cross-correlation comparison with simulated ones. The acquisition time is limited by the capture rate of the CCD camera; amapping of 200 × 200 pixels using a probe size of 10 nmwith a step Fig. 6 Principle of NBD. Scanning a beamthrough a TEM lamella produces a diffraction pattern at each point, which is captured by a CCD camera. The diffraction patterns provide local orientation and phase information on polycrystallinematerials. Fig. 7 NBD line profile through a polysilicon gate. (a) Reference PMOS with different diffraction patterns: multiple grains. (b) Failing PMOS, same diffraction pattern: monograin of polysilicon (b) (a)
Made with FlippingBook
RkJQdWJsaXNoZXIy MjA4MTAy