March_2022_AMP_Digital

A D V A N C E D M A T E R I A L S & P R O C E S S E S | M A R C H 2 0 2 2 2 0 p 361-374, 2006. 2. M. Rappaz, et al., Development of Microstructures in Fe-15Ni-15Cr Single Crystal Electron Beam Welds, Metall Mater Trans A, Vol 20(6), p 1125-1138, 1989. 3. M. Rappaz and C.A. Gandin, Probabilistic Modelling of Microstruc- ture Formation in Solidification Pro- cesses, Acta Mater., Vol 41(2), p 345-360, 1993. 4. M. Henderson, et al., Nickel Based Superalloy Welding Practices for Industrial Gas Turbine Applications, Sci. Technol. Weld. Join., Vol 9(1), p 13-21, 2004. 5. https: //www.mr i .psu.edu/mr i / newspubs/focus-materials/advanced- ma n u f a c t u r i n g / f a s t - %E 2%8 0% 9 3 - p e n n - s t a t e % E 2 % 8 0 % 9 9 s - manufacturing-scale-fast. 6. J. Smith, et al., Linking Process Structure Property and Performance for Metal-Based Additive Manufacturing: Computational Approaches With Ex- perimental Support, Comput. Mech., Vol 57(4), p 583-610, 2016. 7. P. Rangaswamy, et al., Residual Stresses in Components Formed by the Laser-Engineered Net Shaping Process, J. Strain. Anal. Eng. Des., Vol 38(6), p 519-527, 2003. 8. T. DebRoy, et al., Additive Manu- facturing of Metallic Components – Process, Structure and Properties, Prog. Mater. Sci., Vol 92(5), p 112-224, 2018. 9. https://www.totalmateria.com/ page.aspx? ID=CheckAr t icle&s i te= kts&NM=355. 10. A. Basak and S. Das, Additive Manufacturing of Nickel-Base Super- alloy R N5 Through Scanning Laser Epitaxy (SLE) – Material Processing, Microstructures, and Microhardness Properties, Adv. Eng. Mater., Vol 19(3), p 1600690, 2017. 11. P.R. Gradl, et al., Lightweight Thrust Chamber Assemblies Using Multi Alloy Additive Manufacturing and Composite Overwrap, https://www.nasa.gov/sites/ default/files/atoms/files/2020_aiaa_ rampt_multimetallic_compositecham- bers-final.pdf. 12. https: //www. f l ightglobal .com/ analysis/analysis-3d-printing-brings- scramjet-engines-closer-to-reality/ 133652.article. 13. A. Reichardt, et al., Advances in Additive Manufacturing of Metal-Based Functionally Graded Materials, Int. Mater. Rev., Vol 66(1), p 1-29, 2021. 14. V.A. Popovich, et al., Functionally Graded Inconel 718 Processed by Additive Manufacturing: Crystallo- graphic Texture, Anisotropy of Micro- structures and Mechanical Properties , Mater. Des., Vol 114, p 441-449, 2017. 15. L.D. Bobbio, et al., Additive Man- ufacturing of a Functionally Graded Material from Ti-6Al-4V to Invar: Experimental Characterization and Thermodynamic Calculations, Acta Mater., Vol 127, p 133-142, 2017. 16. Y. Chen and F. Liou, Additive Manufacturing of Metal Functionally Graded Materials: A Review, Proc. of the 29 th Annual Int. Solid Freeform Fabrication Symposium, p 1215, 2018. 17. https://techport.nasa.gov/view/ 94980. 18. T.G. Nieh and J. Wadsworth, Recent Advances and Developments in Refractory Alloys, Materials Research Society, Vol 1, 1993. 19. O. Mireles, et al., Additive Manufacturing of Refractory Alloy C103 for Propulsion Applications, AIAA Propulsion and Energy 2020 Forum, https://doi.org/10.2514/6.2020-3500. 20. N.R. Philips, M. Carl, and N.J. Cunningham, New Opportunities in Refractory Alloys, Metall. Mater. Trans. A, Vol 51, p 3299-3310, 2020. different solidification and solid-state transformation routes at the intermedi- ate unicompositional steps. Based on this data, a plan was de- veloped to additively build a graded structure with a defined gradient step size and pathway. Future research in- cludes post-build characterization cou- pled with a fundamental evaluation of phase transformation and deformation mechanisms in these graded structures. This approach provides a critical path toward a broader vision of employing breakthrough AM functionalities with integrated design, manufacturing, and materials evolution criteria. ~AM&P Acknowledgment This work was sponsored by ORNL Director’s Research and Development Fund (#10700) under Strategic Hire Initiative. For more information: Soumya Nag, Materials Science and Technology Di- vision, Oak Ridge National Laboratory, 1 Bethel Valley Rd., Oak Ridge, TN 37830, 865.241.9586, nags@ornl.gov. Notice This manuscript has been au- thored by UT-Battelle LLC, under con- tract DE-AC05-00OR22725 with the U.S. Department of Energy (DOE). The U.S. Government retains and the publisher, by accepting the article for publication, acknowledges that the U.S. government retains a nonexclusive, paid-up, irrevo- cable, worldwide license to publish or reproduce the published form of this manuscript, or allow others to do so, for U.S. government purposes. DOE will provide public access to these results of federally sponsored research in accor- dance with the DOE Public Access Plan (http://energy.gov/downloads/doe- public-access-plan). References 1. T.M. Pollock and S. Tin, Nickel- BasedSuperalloys for AdvancedTurbine Engines: Chemistry, Microstructure and Properties, J. Propuls. Power, Vol 22(2),

RkJQdWJsaXNoZXIy MTMyMzg5NA==