February_EDFA_Digital

edfas.org ELECTRONIC DEVICE FAILURE ANALYSIS | VOLUME 20 NO. 1 20 MICROSTRUCTURE AND RELIABILITY OF TIN-SILVER MICRO-COPPER PILLAR ASSEMBLIES Mohammed Genanu 1 , Babak Arfaei 1 , Eric J. Cotts 1 , Francis Mutuku 1,2 , Eric Perfecto 3 , Scott Pollard 4 , and Aric Shorey 4 1 Physics and Materials Science, Binghamton University, Binghamton, N.Y. 2 Universal Instruments Corporation, Conklin, N.Y. 3 IBM Corporation, Fishkill, N.Y. (now GLOBALFOUNDRIES) 4 Corning Inc., Corning, N.Y. mgenanu1@binghamton.edu EDFAAO (2018) 1:20-31 1537-0755/$19.00 ©ASM International ® T he desire for smaller, lighter, and faster products drives the development of 2.5-D/3-D integration technologies that can use tens of thousands of con- nectionsper die.Micro-copper pillar geometrieshavebeen widely adopted because their small size and fine pitch provide high thermal conductivity, higher input/output (I/O) density, and resistance to deleterious electromigra- tion effects. In micro-copper pillars, SnAg solder is elec- troplated on top of a copper pillar. Because of the small volume of solder employed, intermetallic compounds (IMCs) comprise a significant fraction of the resulting solder joint, and very fine Ag 3 Sn precipitate morpholo- gies can occur. Thus, the microstructure of SnAg solder/ copper pillar microstructures varies significantly from that of larger solder joints, such as flip-chip solder joints. Furthermore, 2.5-D applications include interposers of distinctly different materials, such as silicon or glass. The different properties of thesematerials, such as coefficient of thermal expansion (CTE), affect the thermomechanical response of the package to temperature excursions and the lifetime of the package. Thus, behaviors of copper pillar packages during accelerated thermal cycling (ATC) were examined. Correlations between the shear strength and microstructure of copper pillars were examined for different solder compositions and for different aging times. Microstructure analysis (e.g., Ag 3 Snprecipitatemor- phology) was performed with both optical and scanning electron microscopy (SEM). The effects of thermal aging on the growth of intermetallic compounds, the Ag 3 Sn precipitate morphology, and the mechanical properties of micro-copper pillar bumps were examined. The shear strength performance of micro-copper pillars with three different bump diameters (30, 50, and 100 µm) was also evaluated. Results were considered in terms of variations in the precipitate morphology and in terms of increases in the thicknesses of intermetallic layers at micro-solder/ substrate interfaces. The ATC test results for two different interposers (siliconandglasswithhighCTE) are discussed. INTRODUCTION Varying the processing of lead-free solder joints affects their microstructure and their reliability. Important examples are changes in geometry, solder composition, or thermal history. Each factor can significantly affect solder joint microstructure and lifetime. [1-6] For instance, the number, size, and arrangement of Ag 3 Sn precipitates each affect the mechanical response of near-eutectic Sn-Ag-Cu solder joints and their reliability. [1-8] Geometry is also an important factor. Smaller solder joints undercool more after reflow and solidify at lower temperatures, generally resulting in a more refined microstructure. [9] Thermal history, most importantly aging time, can also significantly affect lead-free solder joint microstructure andmechanical behavior. The Ag 3 Sn precipitates coarsen during aging and lose their effectiveness in hindering the motion of dislocations, particularly aging at elevated temperatures. [10] The present study seeks to better characterize and understand interactions among processing, microstruc- ture, and the properties of lead-free solder joints in copper Originally published in the Proceedings of SMTA International, Sept. 25 ‐ 29, 2016 (Rosemont, Ill.)

RkJQdWJsaXNoZXIy MjA4MTAy